Skip to content
CNC machined metals

Aluminium 5083: marine-grade aluminium

5083 is an aluminium alloy with 4.0 to 4.9% magnesium plus manganese and chromium. It can't be strengthened by heat treatment; its strength comes from the magnesium and from cold working. It resists seawater and industrial chemicals, which makes it a marine favourite.

  • Non-ferrous metal, work-hardened
  • 305 MPatensile strength
  • 2.66 g/cm³density
  • 120 W/m·Kthermal conductivity
Aluminium 50835083Metals
Al-Mg alloy, non-heat-treatable (marine grade)
At a glance

Aluminium 5083 properties

Figures from one named manufacturer or industry data sheet, compared with our other CNC metals. See every material side by side in the property comparison.

Density
2.66 g/cm³
Tensile strength
305 MPa
Stiffness (modulus)
70.3 GPa
Thermal conductivity
120 W/m·K
Melting point (start)
574 °C

Data source: Austral Wright Metals aluminium alloy 5083 (tensile is the H116/H321 minimum). Typical values, not guaranteed minimums.

How it rates for prototyping

  • Clear or see-throughNot suited
  • Living hingeNot suited
  • Heat resistantExcellent
  • Snap fits and clipsPoor
  • Strong and toughVery good
  • Wear resistantLimited
  • Water resistantExcellent
  • Easy to paint or plateVery good
  • Low frictionLimited
  • LightweightGood
  • Conducts heat and electricityVery good
  • Rubber-like and flexibleNot suited
  • Chemical or corrosion resistantVery good

Guide only. General ratings for prototyping, not a recommendation for your application. Filter every material by these needs.

Tensile strength MPa

  • Aluminium 7075570
  • Stainless steel515
  • Brass495
  • Mild steel440
  • Aluminium 6061310
  • Aluminium 5083305
  • Copper210
  • Zinc126

Density g/cm³

  • Copper8.89
  • Brass8.47
  • Stainless steel8.00
  • Mild steel7.87
  • Zinc7.14
  • Aluminium 70752.81
  • Aluminium 60612.7
  • Aluminium 50832.66

Thermal conductivity W/m·K

  • Copper388
  • Aluminium 6061152
  • Aluminium 7075130
  • Brass121
  • Aluminium 5083120
  • Zinc113
  • Mild steel52
  • Stainless steel16
Strengths and limitations

Is Aluminium 5083 right for your part?

Every material has trade-offs. Knowing them up front saves time and money.

Strengths

  • Excellent resistance to seawater and industrial chemicals
  • Very good weldability by TIG and MIG
  • Good ductility for its strength (305 MPa minimum tensile in H116/H321)
  • Light (2.66 g/cm³)

Limitations

  • Machinability rated only "fair", so it is gummier to cut than 6061
  • Not corrosion-proof: pitting, crevice and galvanic corrosion remain possible
  • Not recommended for use above 65 °C
  • Welding softens the heat-affected zone to about annealed strength

Aluminium grades compared

Aluminium 6061Aluminium 7075Aluminium 5083
Tensile strength MPa310570305
Density g/cm³2.72.812.66
Stiffness GPa6871.770.3
Thermal conductivity W/m·K152130120
CharacterGeneral purpose, heat-treatableHigh strengthMarine grade, not heat-treatable
WeldabilityExcellent (MIG, TIG), but welding loses T6 strengthNot arc weldableVery good
Corrosion resistanceExcellentVulnerable to stress-corrosion crackingExcellent in seawater

Typical figures from Wikipedia (6061-T6, 7075-T651) and Austral Wright Metals (5083, H116/H321 minimum); ratings from BlueScope Distribution, The Fabricator, Wikipedia and Austral Wright.

Design tips

Getting the best from Aluminium 5083

Practical points to consider when you design a part in Aluminium 5083.

01

Watch galvanic contact

Where 5083 touches stainless steel or copper in wet conditions, galvanic corrosion is a risk, so such joints are usually insulated.

02

Keep it below 65 °C

Austral Wright advises against using 5083 above 65 °C.

03

Weld it, with care

It welds very well by TIG and MIG, but welding softens the heat-affected zone of H116 and H321 plate to about annealed strength.

Did you know?Magnesium is lighter than aluminium, so the 4 to 5% magnesium in 5083 makes it slightly lighter than 6061 (2.66 against 2.70 g/cm³).
Uses and finishes

Where Aluminium 5083 is used

Marine fittings and structures, unfired welded pressure vessels, transport equipment and offshore structures.

Finishes we offer

  • Machine
  • Bead blast (matt)
  • Brushed
  • Polished
  • Anodised (clear or colour)
  • Painted (including metallic)
  • Powder coated
All surface finishes
FAQ

Common questions

Common questions about Aluminium 5083. Still unsure? Contact us or call +61 3 9764 2749.

Why is 5083 called marine grade?

It resists seawater and industrial chemicals well, which suits boats, offshore and marine structures.

Can 5083 be heat-treated?

No. Its strength comes from magnesium and cold working, not heat treatment.

Is 5083 harder to machine than 6061?

Its machinability is rated "fair", so it is gummier to cut than 6061.

Sources

  1. Property figures: Austral Wright Metals aluminium alloy 5083 (tensile is the H116/H321 minimum)

Please use this information as a guide only. It is a general rapid prototyping reference based on typical results, and many assumptions were made in producing it. It is not a recommendation for any particular application, so please don't use it for product design or engineering decisions. The final choice of process and material is yours; check critical properties with the material manufacturer's data sheets.

Ready to make your part?

Upload your CAD files for a free, obligation-free quote.