Heat treatment of machined steel parts: hardening, tempering, case hardening and stress relief

Many machined steel parts, such as shafts, pins, gears, cams, tooling and wear parts, reach their full performance only after heat treatment. It can make a part several times harder and much stronger, or relieve the stresses that make it move. It also changes dimensions, so it has to be planned together with the machining.

Schematic of a hardening and tempering cycle for steel

What heat treatment does

Steel’s properties depend on its microstructure, and heating and cooling change that structure. Heat treatment uses controlled temperature cycles to make steel harder, stronger, tougher or more stable. The right treatment depends on the steel grade: its carbon and alloy content decide which treatments work and what hardness is possible.

Through hardening and tempering

Heat and soakstructure transformsQuenchhard but brittleTempertoughness restoredTime →Temperature →Schematic only: temperatures and times depend on the steel grade
Hardening and tempering, schematically: heat and soak, quench, then temper. Temperatures and times depend on the grade.

Medium and high carbon steels and many alloy steels can be hardened through their section. The part is heated until its structure transforms, held there, then quenched rapidly in oil, water, polymer or gas. The result is very hard but brittle, so the part is then tempered: reheated to a lower temperature to trade some hardness for toughness. The tempering temperature sets the final balance.

Grades commonly through-hardened include alloy steels such as 4140 and 4340 and tool steels such as O1, D2 and H13. Hardness is usually specified as a Rockwell C range, for example “harden and temper to 40 to 45 HRC”.

Case hardening

Many parts need a hard, wear-resistant surface with a tough core: gears, cams, pins and shafts that see contact wear and shock. Case hardening provides that.

  • Carburising diffuses carbon into the surface of a low-carbon steel at high temperature, then the part is quenched and tempered. The case becomes hard while the low-carbon core stays tough. The case depth is specified on the drawing.
  • Nitriding diffuses nitrogen into the surface at a lower temperature, with no quench. It gives a very hard, thin case with little distortion, so it suits finished, precise parts in suitable alloy and tool steels.
  • Induction hardening heats only selected areas, such as a bearing journal or gear teeth, with an induction coil, then quenches them. The rest of the part is unaffected.

Stress relieving and annealing

Not all heat treatment is about hardness. Stress relieving heats a part below its transformation temperature to relax internal stresses from rolling, welding or heavy machining. It is often done after rough machining on large or asymmetric parts, so that the part does not move during or after finish machining. Annealing softens steel fully for easier machining or forming, and normalising refines the grain structure.

What about stainless steel and aluminium?

Austenitic stainless steels such as 304 and 316 cannot be hardened by heat treatment; they gain strength only by cold work. Martensitic grades such as 420 and 440C can be hardened, and precipitation-hardening grades such as 17-4PH are aged to a range of strength levels. Aluminium alloys such as 6061 and 7075 are supplied already heat treated, typically in the T6 condition. Heating them, including by welding, reduces that strength.

Distortion: plan the sequence

Hardening, and quenching in particular, changes the size and shape of a part. It can grow, shrink, bow or go out of round, and the amount depends on the grade, geometry and process. Thin sections next to thick ones and asymmetric parts distort most. Through-hardened steel is also much harder to machine afterwards. A typical sequence for precise hardened parts is:

  • Rough machine, leaving stock on precision features.
  • Stress relieve if the part is large or asymmetric.
  • Finish machine the features that are not critical after hardening.
  • Heat treat.
  • Grind or hard-machine the precision features (bearing seats, bores, sliding faces) to final size.

Nitrided parts, with very low distortion, are often finish machined before treatment. Threads are usually cut before hardening and may need masking or a check afterwards.

Design for heat treatment

  • Keep section thickness as uniform as practical, and avoid sharp internal corners, which concentrate stress and can crack during quenching.
  • Give generous radii at shoulders and grooves on shafts.
  • Avoid holes close to edges in parts that will be through-hardened.
  • Allow grinding stock on precision features.
  • Mark areas that must stay soft, for example for later drilling or peening; they can be masked during carburising.

How to specify heat treatment

What to stateExample
Steel grade and condition as supplied4140, annealed or pre-hardened
TreatmentHarden and temper; carburise; nitride; induction harden; stress relieve
HardnessRange and scale, such as HRC
Case depth (case hardening)Effective case depth and the hardness at which it is measured
Areas to treat or maskIndicated on the drawing
SequenceFeatures to be finished after heat treatment

Tell us the grade and the hardness or treatment you need when you request a quote, and we arrange the heat treatment as part of the job, with machining sequenced around it.

CNC machined steel parts
Machined steel parts: many reach full performance only after heat treatment.
CNC machined shaft and link part
Shafts like this are commonly hardened on bearing journals and then ground.
FAQ

Common questions

Still unsure? Contact us or call +61 3 9764 2749.

Can mild steel be hardened?

Low-carbon mild steel does not through-harden significantly, but it can be case hardened by carburising, which gives a hard surface and a tough core.

Can 304 or 316 stainless steel be heat treated to harden it?

No. Austenitic stainless steels gain strength only by cold work. Martensitic grades such as 420 and precipitation-hardening grades such as 17-4PH can be hardened.

Should a part be machined before or after hardening?

Usually it is rough and semi-finish machined before hardening, then precision features are ground or hard-machined after, because hardening causes some distortion.

How is hardness specified on a drawing?

As a range on a stated scale, usually Rockwell C for hardened steels, for example 40 to 45 HRC. For case hardening, also give the effective case depth.

Ready to make your part?