Skip to content
Comparisons

Aluminium 6061 vs 7075: strength, stiffness, corrosion and cost

Aluminium 6061 and 7075 are the two alloys most often specified for machined aluminium parts. 7075 is far stronger; 6061 is more versatile, more corrosion resistant, weldable and less expensive. Knowing exactly where they differ, and where they do not, avoids paying for strength you do not need or running short of it where you do.

CNC machined aluminium parts with a blue anodised finish

Two alloy families

6061 is an aluminium-magnesium-silicon alloy (6000 series). It is the general-purpose structural alloy: good strength, very good corrosion resistance, weldable, and easy to machine and anodise. 7075 is an aluminium-zinc alloy with magnesium and copper (7000 series), developed for aircraft structures. It is one of the strongest aluminium alloys in common use. Both are usually machined in the T6 temper: solution heat treated and artificially aged.

Properties side by side

6061-T67075-T6Tensile strengthMPa310570Yield strengthMPa276503HardnessBrinell95150Elastic modulusGPa6871.7Densityg/cm³2.72.81Thermal conductivityW/m·K152130Typical values for T6 temper
Typical properties of 6061-T6 and 7075-T6. Bars are scaled within each row.
Typical published values; check the data sheet for your supplier and temper.
Property (typical, T6)6061-T67075-T6
Tensile strength310 MPa570 MPa
Yield strength276 MPa503 MPa
Elongation at breakabout 12%about 11%
Fatigue strengthabout 97 MPaabout 159 MPa
Hardnessabout 95 HBabout 150 HB
Elastic modulus68 GPa71.7 GPa
Density2.70 g/cm³2.81 g/cm³
Thermal conductivity152 W/m·K130 W/m·K
WeldabilityGoodNot suitable for arc welding
Corrosion resistanceVery goodModerate

Strength: 7075 is in a different league

7075-T6 has roughly 80 percent more tensile and yield strength than 6061-T6, and much better fatigue strength. For highly stressed parts, such as gears, shafts, keys, aircraft fittings, highly loaded motor mounts and bicycle components, that margin allows lighter sections or a higher safety factor. Its higher hardness also helps with wear and dents.

Stiffness: no meaningful difference

This is the point most often missed. The elastic modulus of 7075 is only about 5 percent higher than 6061. If a part is deflecting too much, changing from 6061 to 7075 will barely help; it will just make the part stronger at the same deflection. To make an aluminium part stiffer, change its geometry: deeper sections, ribs, shorter spans. Strength and stiffness are different properties.

Corrosion and environment

6061 has very good general corrosion resistance and is widely used outdoors and in marine-adjacent environments, usually anodised or painted. The copper in 7075 lowers its corrosion resistance, and in the T6 temper it is susceptible to stress corrosion cracking when stressed in a corrosive environment. Over-aged tempers such as T73 trade some strength for much better resistance. 7075 parts are typically protected by anodising or painting.

Welding

6061 is readily weldable, although the heat-affected zone loses a substantial part of its T6 strength unless the assembly is heat treated again. 7075 is generally regarded as unsuitable for arc welding because it is prone to cracking. Parts in 7075 are joined mechanically: bolts, pins, rivets or adhesive bonding.

Machining and anodising

Both alloys machine well. The harder 7075 tends to give a fine finish and well-broken chips, and holds small features crisply. 6061 machines easily too and is generally lower in material cost. Both can be anodised, clear or coloured, and both can be hard anodised: a thicker, harder oxide layer for wear and abrasion resistance, used on sliding parts, pistons, gears and parts that see knocks. Hard anodising grows partly outwards from the surface, so allow for it on tight fits and threads. 6061 gives very consistent clear and coloured anodising; on 7075 the clear finish can look slightly different in tone, and colours can vary a little between alloys and batches, so if two alloys sit side by side in an assembly, test the match. Our anodising article explains the process.

CNC machined aluminium parts anodised blue
Machined aluminium with a blue anodised finish.

Cost and availability

7075 costs more per kilogram than 6061 and is stocked in a narrower range of sizes in some markets. For most machined parts the difference in part price is modest, because machining time dominates, but on large or bulky parts the material cost difference is noticeable.

Which is commonly used where?

Typically 6061Typically 7075
Brackets, housings and enclosuresHighly stressed brackets and fittings
Jigs, fixtures and machine partsGears, shafts, keys and worm gears
Heat sinks and thermal partsAerospace and defence structural parts
Welded frames and structuresLightweight high-strength sporting parts
Outdoor and marine-adjacent partsParts where weight must be minimised at a given strength

As a general pattern: 6061 is the default, and 7075 is chosen when a strength calculation shows 6061 does not have enough margin, and welding is not needed. Our material pages for 6061, 7075 and 5083 give sourced data, and our property comparison charts them against other materials.

Because CNC machining needs no mould or die, the program that made your prototypes can also make the production batch. Runs of a few hundred parts go straight from approved prototype to production in the real engineering material, and a design change is a program edit rather than a new tool.

FAQ

Common questions

Still unsure? Contact us or call +61 3 9764 2749.

Is 7075 stronger than 6061?

Yes. In the T6 temper, 7075 has about 570 MPa tensile strength against about 310 MPa for 6061, and much higher yield and fatigue strength.

Is 7075 stiffer than 6061?

Only very slightly. Their elastic moduli are about 72 and 68 GPa. To make a part stiffer, change the geometry rather than the alloy.

Can 7075 be welded?

7075 is generally regarded as unsuitable for arc welding because it is prone to cracking. 6061 is readily weldable, with some strength loss near the weld.

Can both alloys be anodised?

Yes. Both can be clear or colour anodised, and both can be hard anodised for wear resistance. Colours can vary slightly between alloys and batches, so test the match if both are used side by side.

Ready to make your part?

Upload your CAD files for a free, obligation-free quote.